中空玻璃双组份打胶机使用不正常了怎么办

时间:2022-05-23 来源:http://www.jncsjx.com/ 发布人:昌盛机械

在使用玻璃打胶机的过程当中会遇到各种各样的问题,那么卧式玻璃打胶机的中空胶拉断时间不正常了怎么办呢?下面我们来一一向您介绍。
Various problems will be encountered in the process of using the glass gluing machine. What if the hollow glue breaking time of the horizontal glass gluing machine is abnormal? Now let's introduce to you one by one.
一般致断中空胶拉断时间过长过短的时间一般主要是由以下四类原因所引起的:环境温度偏高会导致拉断时间变短,环境温度偏低会导致拉断时间延长;环境湿度过低也会导致拉断时间有所延长。解决方法:采取空调、暖房、晒水等方法让使用环境和养护环境的温湿度在合适范围内。
Generally, the breaking time of hollow glue is too long and too short, which is mainly caused by the following four reasons: the high ambient temperature will lead to the shortening of the breaking time, and the low ambient temperature will lead to the prolongation of the breaking time; Too low ambient humidity will also lead to an extension of the breaking time. Solution: adopt air conditioning, greenhouse, water drying and other methods to keep the temperature and humidity of the use environment and maintenance environment within the appropriate range.
B组份比例太高会导致拉断时间变短,B组分比例偏低会导致拉断时间延长。解决方法:调节中空胶的A、B组分配比使其在中空胶制造商要求的范围内。
Too high proportion of component B will shorten the breaking time, and too low proportion of component B will prolong the breaking time. Solution: adjust the distribution ratio of group A and group B of hollow rubber to make it within the range required by the hollow rubber manufacturer.


夏季配方的胶在冬季使用时,环境温度下降,拉断时间会偏长;而冬季配方的胶在夏天使用,由于环境温度上升,拉断时间会缩短。解决方法:冬、夏季用胶时尽量选用相对应季节配方的中空胶。
When the glue formulated in summer is used in winter, the ambient temperature decreases and the breaking time will be too long; The glue formulated in winter is used in summer, and the breaking time will be shortened due to the rise of ambient temperature. Solution: when using glue in winter and summer, try to use hollow glue with corresponding seasonal formula.
污染物的影响。比如打胶机之前使用的是其他类型或其他的中空胶,换胶后由于打胶机清洗不干净,拉断时间会有影响。尤其是打胶机之前使用的是聚硫胶,换用硅酮胶,如果打胶机没有完全清洗干净,拉断时间会明显变长。解决方法:换胶时,一定要将打胶机及管道清理干净;尤其是之前使用的是聚硫换用硅酮胶,一定要将设备所有物料流道相关部件完全拆卸,用合适的溶剂完全将残余物料清洗干净,即使很少量的聚硫胶残余都会造成硅酮胶的拉断时间明显延长。
Impact of pollutants. For example, the glue applicator used hollow glue of other types or brands before. After changing the glue, the breaking time will be affected due to the unclean cleaning of the glue applicator. In particular, polysulfide glue is used before the gluing machine, and silicone glue is used instead. If the gluing machine is not completely cleaned, the breaking time will be significantly longer. Solution: when changing the glue, be sure to clean the glue applicator and pipeline; In particular, the previous use of polysulfide is to replace silicone adhesive. All relevant parts of the material flow path of the equipment must be completely disassembled and the residual materials must be completely cleaned with appropriate solvent. Even a small amount of polysulfide adhesive residue will significantly prolong the breaking time of silicone adhesive.
本文的精彩内容由中空玻璃丁基胶涂布机提供知识提供,本网站还有很多的精彩内容,更多的内容您可以点击进入:http://linshi.jncsjx.com我们有专门的客服为您解答问题
The wonderful content of this article is provided by the insulating glass butyl adhesive coater. There are many wonderful contents on this website. You can click to enter more contents: http://linshi.jncsjx.com We have special customer service to answer your questions

联系我们Contact us

  • 咨询热线:0531-85717458 13705446998
  • 公司地址: 山东省德州市齐河安头乡企巢工业园
  • 扫码联系我们:

截屏,微信识别二维码

微信号:13705446998

//